良好的柔韧性,耐热性,高,电缆护套,电线电缆应用FEP CJ-95

 

Teflon® FEP CJ-95
聚全氟乙烯-丙烯树脂
DuPont Fluoropolymers

产品说明

DuPont™ Teflon® FEP CJ-95 is a melt-processible fluoropolymer resin specifically designed for cable insulation and jacketing applications that demand a high degree of stress crack resistance.

This resin provides the electrical and mechanical properties needed for low-voltage applications. Teflon® FEP CJ-95 has a higher melt flow rate than Teflon® FEP 140, but it retains similar stress crack resistance.

Like all Teflon® fluoropolymer resins, Teflon® FEP CJ-95 offers an excellent combination of properties: chemical inertness, exceptional dielectric properties, heat resistance, toughness, flexibility, low coefficient of friction, nonstick characteristics, negligible moisture absorption, low flammability, performance at temperature extremes, and weather resistance.

总体

材料状态 • 已商用:当前有效   
供货地区 • 北美洲 • 欧洲  
 • 南美洲 • 亚太地区  
    
 • 低摩擦系数 • 耐气候影响性能良好 • 吸潮性差 
性能特点 • 良好的柔韧性 • 耐热性,高  
   • 阻燃性能 
 • 耐化学性良好 • 韧性良好  
    
用途 • 电缆护套 • 电线电缆应用 • 绝缘材料 
形式 • 颗粒料   
加工方法 • 挤出   

物理性能 额定值单位制 测试方法
比重 2.14g/cm³ ASTM D792
熔流率 (372°C/5.0 kg) 5.0g/10 min ASTM D1238
机械性能 额定值单位制 测试方法
抗张强度 26.0MPa ASTM D638
伸长率 (断裂) 300% ASTM D638
硬度 额定值单位制 测试方法
硬度计硬度 (邵氏 D) 55 ASTM D2240
热性能 额定值单位制 
熔融温度 254°C 
电气性能 额定值单位制 测试方法
介电强度  ASTM D149
0.254 mm 79kV/mm 
3.18 mm 20kV/mm 
介电常数  ASTM D150
100 kHz 2.02 
1 MHz 2.02 
耗散因数 (1 MHz) 0.00070 ASTM D150
补充信息  
Specific Gravity, ASTM D792: 2.12 to 2.17  
  
挤出 额定值单位制 
第1气缸区温度 366°C 
第2气缸区温度 382°C 
第3气缸区温度 391°C 
第4气缸区温度 396°C 
第5气缸区温度 396°C 
连接器温度 396°C 
熔体温度 404°C 